Langmuir-Blodgett films in high-pressure rolling contacts
Langmuir-Blodgett films in high-pressure rolling contacts
Ultrathin film interferometry has been used to measure the film thickness of deposited Langmuir-Blodgett layers of stearic acid in a rolling, high pressure, ball on flat contact.
Deposited multilayers up to five monolayers thick have been found to remain in a vertically-oriented configuration in static contact up to Hertzian pressures of at least 0.7 GPa. It has been shown that one deposited monolayer is extremely durable in rolling conditions and continues to show a thickness of at least 2 nm (the vertically-oriented monolayer) even at high speeds and in the presence of supernatant hydrocarbon solvent. Multilayers showed variable behavior. Two monolayers rapidly reduced to one, while three initial monolayers stabilized after rolling at a film thickness corresponding to between one and two monolayers. A four monolayer initial film reduced only slightly in thickness during rolling, to reach a level corresponding to three monolayers.
The results have been interpreted in terms of the transfer of one or more deposited molecular layers from the disc to the ball surface
24-30
Ratoi, M.
cfeffe10-31ca-4630-8399-232c4bc2beff
Spikes, H.A.
e8d32127-b018-44b9-ad78-49e446ed590e
Bovington, C.
74d94506-5396-4898-852d-d38924bdaa1e
25 January 2003
Ratoi, M.
cfeffe10-31ca-4630-8399-232c4bc2beff
Spikes, H.A.
e8d32127-b018-44b9-ad78-49e446ed590e
Bovington, C.
74d94506-5396-4898-852d-d38924bdaa1e
Ratoi, M., Spikes, H.A. and Bovington, C.
(2003)
Langmuir-Blodgett films in high-pressure rolling contacts.
Tribology Transactions, 46 (1), .
(doi:10.1080/10402000308982595).
Abstract
Ultrathin film interferometry has been used to measure the film thickness of deposited Langmuir-Blodgett layers of stearic acid in a rolling, high pressure, ball on flat contact.
Deposited multilayers up to five monolayers thick have been found to remain in a vertically-oriented configuration in static contact up to Hertzian pressures of at least 0.7 GPa. It has been shown that one deposited monolayer is extremely durable in rolling conditions and continues to show a thickness of at least 2 nm (the vertically-oriented monolayer) even at high speeds and in the presence of supernatant hydrocarbon solvent. Multilayers showed variable behavior. Two monolayers rapidly reduced to one, while three initial monolayers stabilized after rolling at a film thickness corresponding to between one and two monolayers. A four monolayer initial film reduced only slightly in thickness during rolling, to reach a level corresponding to three monolayers.
The results have been interpreted in terms of the transfer of one or more deposited molecular layers from the disc to the ball surface
Text
LB Films in High Presurre Rolling Contacts.pdf
- Version of Record
Restricted to Repository staff only
Request a copy
More information
Published date: 25 January 2003
Organisations:
nCATS Group
Identifiers
Local EPrints ID: 356063
URI: http://eprints.soton.ac.uk/id/eprint/356063
ISSN: 1040-2004
PURE UUID: a5b38fa4-871c-4efc-83a3-04ce8a5a8c6b
Catalogue record
Date deposited: 25 Oct 2013 14:09
Last modified: 15 Mar 2024 03:35
Export record
Altmetrics
Contributors
Author:
H.A. Spikes
Author:
C. Bovington
Download statistics
Downloads from ePrints over the past year. Other digital versions may also be available to download e.g. from the publisher's website.
View more statistics