The evolution of break arc erosion from arc initiation to extinction on silver alloy electrical contacts in low voltage DC switches
The evolution of break arc erosion from arc initiation to extinction on silver alloy electrical contacts in low voltage DC switches
This study concerns the evolution of electrical contact erosion in low voltage 42V DC (24A) applications. The aim is to describe the erosion mechanisms of a single arc discharge at both contact surfaces during operation. To this end the experiments conducted are designed to produce results that enable close examination of the surface profile changes, volumetric contact material movements, and relative quantities of metallic and gaseous species in the arc discharge.
The experimental procedure is arranged so that the contacts undergo a low number of operation cycles in order to limit the cumulative effects of arc erosion. To obtain results portraying the evolution of arc erosion in a 42V system the apparatus allows for interruption of the arc at any desired voltage level. A series of tests are conducted at specified voltage steps from arc initiation to extinction.
The samples collected are analysed using a non-contact laser profile apparatus giving 2D and 3D surface scans. During each arc discharge a record of spectral emissions is collected by a spectrometer and later analysed to show the constituents of the arc.
The data is represented with reference to voltage level and shows how the erosion evolution from a low number of operation cycles is related to arc phenomena. In addition the voltage profiles of the arc are recorded and represented by amplitude modulation. It has been found that the erosion site dimensions are related to the arc voltage fluctuations. In these tests a marked change of voltage slope is seen but is not found to be related to the metallic to gaseous phase transition as often thought.
It is determined that the anodic to cathodic arc transition is not due to a metallic to gaseous phase transition.
Changes in surface profile at the cathode occurring during the cathodic arc phase, and before gaseous phase initiation, are affected by density per unit area of ions impacting the surface. The vaporization of the cathode requires a critical ion density. This determines the anodic to cathodic transition point.
Conversely the anode is thought to endure intense electron sputtering throughout the arc lifetime and its volumetric loss is greater than that of the cathode.
Sumption, Alan
d344b53d-01e1-47b7-80eb-5c8635f4d42f
2005
Sumption, Alan
d344b53d-01e1-47b7-80eb-5c8635f4d42f
Sumption, Alan
(2005)
The evolution of break arc erosion from arc initiation to extinction on silver alloy electrical contacts in low voltage DC switches.
University of Southampton, School of Engineering Sciences, Doctoral Thesis, 228pp.
Record type:
Thesis
(Doctoral)
Abstract
This study concerns the evolution of electrical contact erosion in low voltage 42V DC (24A) applications. The aim is to describe the erosion mechanisms of a single arc discharge at both contact surfaces during operation. To this end the experiments conducted are designed to produce results that enable close examination of the surface profile changes, volumetric contact material movements, and relative quantities of metallic and gaseous species in the arc discharge.
The experimental procedure is arranged so that the contacts undergo a low number of operation cycles in order to limit the cumulative effects of arc erosion. To obtain results portraying the evolution of arc erosion in a 42V system the apparatus allows for interruption of the arc at any desired voltage level. A series of tests are conducted at specified voltage steps from arc initiation to extinction.
The samples collected are analysed using a non-contact laser profile apparatus giving 2D and 3D surface scans. During each arc discharge a record of spectral emissions is collected by a spectrometer and later analysed to show the constituents of the arc.
The data is represented with reference to voltage level and shows how the erosion evolution from a low number of operation cycles is related to arc phenomena. In addition the voltage profiles of the arc are recorded and represented by amplitude modulation. It has been found that the erosion site dimensions are related to the arc voltage fluctuations. In these tests a marked change of voltage slope is seen but is not found to be related to the metallic to gaseous phase transition as often thought.
It is determined that the anodic to cathodic arc transition is not due to a metallic to gaseous phase transition.
Changes in surface profile at the cathode occurring during the cathodic arc phase, and before gaseous phase initiation, are affected by density per unit area of ions impacting the surface. The vaporization of the cathode requires a critical ion density. This determines the anodic to cathodic transition point.
Conversely the anode is thought to endure intense electron sputtering throughout the arc lifetime and its volumetric loss is greater than that of the cathode.
This record has no associated files available for download.
More information
Published date: 2005
Organisations:
University of Southampton
Identifiers
Local EPrints ID: 47499
URI: http://eprints.soton.ac.uk/id/eprint/47499
PURE UUID: 6ba9c1d3-3950-4267-99c8-79169d97d7ae
Catalogue record
Date deposited: 07 Aug 2007
Last modified: 11 Dec 2021 16:41
Export record
Contributors
Author:
Alan Sumption
Download statistics
Downloads from ePrints over the past year. Other digital versions may also be available to download e.g. from the publisher's website.
View more statistics